What Is Color Fastness? Two Scales, One Order Line
Color fastness is how well a dye stays where it was put.
The word covers five different tests, and two different scales. That is why two mills can both say “grade 4” and mean unrelated things.
This page gives the definition, then the numbers behind it. The washing table, the rubbing force in newtons, and the eight-step light scale.
Then it turns all of it into one line you can add to the order.
The Short Answer
Color fastness is the resistance of a dyed or printed textile to losing its color, or to passing it to something else.
The loss can come from washing, rubbing, light, sweat, sea water or pool water. Each has its own test, and its own number.
Two results come out of every test. One is the change in color of the sample itself. The other is staining: how much color moved onto a white cloth held against it.
A result is written as two grades, not one. “4 for change, 3-4 for staining on nylon” is a real result. “Grade 4” on its own is not.
Two Scales, Not One
Washing, rubbing, sweat, sea water and pool water are all graded on a grey scale that runs from 1 to 5. Grade 5 means no change at all.
The grey scale comes in two versions. One judges change in color on the sample. The other judges staining on the white cloth. They are separate standards, and a report should say which one was used.
Half steps exist. A result of 4-5 sits between 4 and 5, and the difference matters when a buyer’s limit is 4.
Light is the exception. Light fastness is graded from 1 to 8 against blue wool references, not on the grey scale at all.
That single fact ends a lot of arguments. A buyer who asks for “grade 7” on a washing test is asking for something the scale cannot give.
Both scales are read by eye against a chart, or by a spectrophotometer that outputs the same grade. The eye method is still the reference method.
Washing: Sixteen Procedures, Not One
Washing fastness is the one most orders name, and the one most buyers under-specify. The standard does not contain one washing test. It contains sixteen.
The sixteen procedures sit in the washing part of the standard. Each one is a letter and a number. A is the mildest, at 40 degrees. E is the harshest, at 95 degrees, the temperature used for hotel and hospital linen.
The suffix tells you how many washes are simulated. S is a single wash. M is a multiple wash, which the standard says can stand in for up to five washes at or below 70 degrees.
The rest of the recipe is fixed too. Detergent goes in at 4 grams per litre. Steel balls, about 6 mm across, add the rubbing action; the mildest test uses 10 and the harshest multiple test uses 100.
Liquor volume drops as temperature rises: 150 ml in the 40 and 50 degree tests, 50 ml above that. From 60 degrees upward the pH is adjusted to 10.5.
| Test | °C | min | Balls | Use |
|---|---|---|---|---|
| A1S | 40 | 30 | 10 | Gentle home wash |
| A1M | 40 | 45 | 10 | Five gentle washes |
| A2S | 40 | 30 | 10 | Home wash with bleach |
| B1S | 50 | 30 | 25 | Warm home wash |
| C1S | 60 | 30 | 25 | Hot home wash |
| C1M | 60 | 45 | 50 | Five hot washes |
| C2S | 60 | 30 | 25 | Hot wash with bleach |
| D1S | 70 | 30 | 25 | Heavy domestic wash |
| E1S | 95 | 30 | 25 | Hospital and hotel linen |
| E2S | 95 | 30 | 25 | Linen with bleach |
Ten of the sixteen are above. The rest add chlorine bleach at 0.015 percent available chlorine, or sit at 70 and 95 degrees with perborate.
The machine matters as much as the recipe. Containers are 75 mm across and 550 ml in volume, and the shaft turns at 40 turns a minute.
That is why two labs in different countries can disagree on a sample without either being wrong. A different machine, a different detergent, a different number of balls: a different result.
Ask which procedure was run before you compare two reports. The procedure number is the only part that makes a washing grade comparable.
Rubbing: Nine Newtons And 104 Millimetres
Rubbing fastness, often called crocking, answers a simple question. If the fabric is rubbed against something white, does color move?
The test uses a crockmeter: a small arm that rubs a white cloth across the sample. The numbers are fixed, which is what makes the result repeatable.
The arm presses down with 9 newtons, give or take 0.1. Each stroke is 104 mm long, give or take 3. Ten strokes go by in ten seconds.
The test runs twice, once with a dry cloth and once with a wet one. The wet result is always the lower of the two, and it is the one that decides returns.
Here the two big standards diverge. The ISO wet test wets the cloth to about 100 percent pickup. The American test uses about 65 percent.
So a sample that passes the ISO version will usually pass the American one, and not the other way round. A mill that quotes one number for both is quoting one number too few.
Trade practice gives a rough guide. Light colours are usually asked for grade 4 or better, dry and wet.
Dark reactive-dyed cotton is the hard case. Wet rubbing of 2-3 is accepted in much of the trade, and 3 or better is treated as good.
If a dark shade comes back at 2, the dyeing was probably not soaped off well enough. A softener can also loosen dye at the surface.
Light: Blue Wool And A Red Cloth
Light fastness is graded on a different ruler. The sample is exposed to a xenon arc lamp that mimics daylight, and compared with eight blue wool references.
Grade 1 fades fastest. Grade 8 barely fades at all. The sample is placed beside the references until it has faded by the same amount as one of them.
That gives a rough map for buyers. Grades 1 to 3 suit indoor goods that see little sun. Grades 4 to 5 are where most apparel brands set their entry level. Grades 6 to 8 belong to outdoor fabric.
One control variable decides more arguments than the lamp itself: humidity inside the chamber. The standard requires a red control cloth to be exposed with the samples to keep it in check.
When humidity drifts high, moisture-sensitive dyes fade faster and the result reads low. That is a lab problem, not a fabric problem, and it is worth asking about.
Sweat, Sea Water And Pool Water
Three more tests matter for anything worn against skin or used near water. None of them can be predicted from a washing result.
A testing company’s summary of the method family lists them all with their standard numbers.
Sweat fastness uses two test liquids, one acid and one alkaline, built around histidine, an amino acid found in perspiration. The sample sits between plates, then dries slowly.
Acid and alkaline results are reported separately, because a dye can hold on in one and let go in the other. A single “sweat 4” hides which one was tested.
Sea water fastness soaks the sample for 30 minutes, presses it at 12.5 kPa and holds it at 37 degrees for four hours before grading.
Pool water fastness uses chlorinated water. Swimwear is tested at 50 or 100 milligrams of chlorine per litre; accessories such as beach robes and towels at 20.
Anything sold as swimwear needs the chlorine test. For hotel and resort pools, ask for the 100 mg/l version.
What A Report Has To Name
A test report is not a certificate. It is a record of what was done, and the standard lists ten things it must state.
The first is the standard and its year, such as ISO 105-C06:2010. Without a year, the report can refer to a method that has since changed.
Then the sample, identified well enough to match a dye lot. Then the grades: change in color, and staining for each fibre strip, not one average.
The method number comes next: A1S, C2S, or whichever was run. Then whether steel balls were used, and whether a souring step followed the wash.
The detergent has to be named too. The standard allows an American reference detergent or a European one, and they do not behave the same.
Last is any difference from the method. A lab that ran 25 minutes instead of 30 is telling you something useful, provided it writes it down.
A report missing the method number, the detergent and the per-fibre staining is not a weak report. It is a report you cannot compare with anything.
Which Test Catches Which Failure
Most complaints arrive as a photo and a sentence. The useful move is to name the test that would have caught it before shipment.
The table below pairs the everyday complaint with the method. It also lists what is usually missing from the order, which is why the complaint arrives at all.
| Product | Complaint | Test that catches it | Missing from the PO |
|---|---|---|---|
| Hotel and hospital linen | Grey or yellow after industrial wash | Washing, E1S or E2S | The method number |
| Dark cotton tee | Colour rubs onto a white bag | Rubbing, wet and dry | Which of the two was tested |
| Curtains and blinds | Faded panel after one summer | Light, xenon arc | The blue wool grade |
| Swimwear | Fading after a hotel pool | Chlorinated water | The chlorine level used |
| Sportswear | Staining under the arms | Perspiration, acid and alkaline | The second of the two results |
| Printed polyester | Colour on the nylon strip | Washing with multifibre strip | Which fibre stained |
None of the right-hand column needs a lab to fix. Each one is a sentence added to the order before the mill starts dyeing.
Where Orders Break
The failures cluster around four process steps. Knowing them helps a buyer ask a question that a mill can actually answer.
The first is washing after dyeing. Reactive dyes need a proper soaping and rinsing cycle to clear the unfixed dye from the fibre surface.
Skip it and the surface dye moves easily. That shows up as low wet rubbing and as staining on the multifibre strip.
The second is heat. A high heat-setting temperature can push dye from inside the fibre to the surface, which spoils rubbing and washing at the same time.
The third is softeners and finishing agents. They improve hand feel and can loosen dye at the surface, so a fabric that passed before finishing can fail after it.
The fourth is fibre choice. Disperse dyes have a strong liking for polyamide, so a nylon strip in the multifibre fabric is often the first place a problem appears.
Weight plays a part too, because a heavier fabric carries more dye per square metre. The weight the mill quotes in grams is worth writing beside the shade reference.
The Order Line
One line, six parts. Method and year, condition letter, the two grades, direction, fibre, and who pays for the test.
Written out, it looks like this. Washing fastness to ISO 105-C06:2010, method C2S, change 4 or better, staining 3-4 or better on each fibre.
For rubbing, add the direction. Twill and satin behave differently along warp and weft, so the standard asks for both directions to be tested.
For light, the grade is blue wool, not grey scale, and the buyer should say so to avoid a report that mixes the two.
Then decide who pays. Lab fees sit in the sample cost, and a mill quoting a price before a test has been agreed is quoting a guess.
Keep the report with the shipment. The inspection that checks a dye lot can confirm shade against the approved standard, but it cannot grade fastness on site.
A loading check cannot grade a dyed lot either, and it is not meant to; what a pre-shipment check covers is defect counting, not chemistry.
So the test report is the only evidence you will have. Put it on one page the mill can sign, together with the shade and the weight.
Send me the fastness line from your order sheet, or the last test report you were given. I will check whether the method, the condition and the two grades can be compared with anything, and which fibre strips were left out. No cost, no obligation.
Check My ClauseQuestions Buyers Ask
What does color fastness mean in plain terms?
How well a dye stays in the fabric. It covers fading of the sample and colour moving onto anything held against it, under washing, rubbing, light, sweat or water.
Is grade 5 the best result?
For washing, rubbing and sweat, yes: the grey scale runs 1 to 5 and 5 means no change. For light fastness the scale runs 1 to 8 against blue wool, so 8 is the best.
Why do ISO and AATCC results differ?
The recipes differ. The ISO wet rubbing test uses about 100 percent moisture pickup, the American test about 65 percent, so the ISO version is harder to pass.
What is a good rubbing result for black cotton?
Trade practice treats wet rubbing of 2-3 as acceptable on dark reactive-dyed cotton, and 3 or better as good. Light colours are usually held to 4 or better.
Do I need every test for every product?
No. Match the test to the use: chlorine for swimwear, light for curtains, perspiration for anything worn against skin, washing for linen that goes through an industrial cycle.
Can a factory self-test and send its own report?
It can, and many do. Ask which machine and which detergent were used, and whether the lab is accredited for that method. A report without those details cannot be compared.
Questions & Comments
We read every one and reply within 24 hoursHas a mill sent you a fastness grade with no method behind it? Paste the line and I will say what is missing before you approve the bulk.