What Is Polypropylene: The Grade Behind The Resin Code
Polypropylene is a semi-crystalline plastic made by joining propylene into long chains. It is light, stiff, heat resistant and cheap, and it is the second most produced plastic in the world.
The word on a drawing is not a spec. Two parts can both say PP and behave very differently at the press.
This page covers four things. What the chain is, how to read a grade, how much the part will shrink, and what food grade really asks for.
The Short Answer
Propylene is a small molecule: three carbon atoms and six hydrogen atoms. Under heat and a catalyst, thousands of them join head to tail.
The chain that comes out has a methyl group on every other carbon. That small side group is why the resin is stiffer and holds heat better than polyethylene.
Most trade PP is isotactic, so the methyl groups sit on the same side of the chain. That regularity lets the chains pack into crystals.
The numbers behind that packing are worth knowing. Industrial grades run 30 to 60 percent crystalline. The isotactic share is usually 85 to 95 percent. It is measured by what stays undissolved in boiling heptane.
Density is where PP wins on freight and on resin cost. References give 0.895 to 0.93 grams per cm3, and a sheet datasheet for a homopolymer prints 0.905.
That is the lowest density in the commodity group. It is why a PP crate is lighter than the same crate in most other resins.
The melting point sits in a band rather than on a point. The US food contact rule prints 160 to 180 degrees Celsius for the grade it covers, and a trade homopolymer datasheet prints 163.
None of that tells you which grade you were quoted. For that you need three rows of a data sheet. They are the subject of the next section.
Why Density Changes The Price Of A Part
Resin is sold by weight and parts are sold by volume. That gap is where density turns into money.
One kg of PP at 0.905 takes up about 1,105 cm3. A 20 cm3 part therefore weighs about 18 grams, and a thousand of them weigh 18 kg.
Move the same part to a resin at 1.2 grams per cubic centimetre and the shipment grows by a third. Nothing about the part changed except the resin.
That arithmetic is also why thin-wall parts are common in this family. Wall stiffness falls with the cube of thickness, so a wall can usually be thinner than the first drawing shows.
Thin walls bring their own problem, and it shows up as a size one. The next two sections deal with it. Shrinkage decides whether the tool is right.
Three Grades, And The Row That Names Them
Under one trade name there are three resins. They differ in what is added to the chain, and the difference reaches the drawing.
Homopolymer. Propylene only. It is the stiffest of the three and the most heat resistant, and it is the one that goes brittle near freezing.
Impact copolymer. A rubber phase of ethylene and propylene is built into the particle. The trade is stiffness for toughness, and the gain is large.
Random copolymer. Ethylene sits inside the chain rather than in a separate phase. Crystallinity drops, the melting point falls, and the part comes out clearer.
The fastest way to tell them apart is one row of a data sheet. Notched Izod impact is measured the same way for all three, so the numbers can be compared directly.
| Grade | What differs | Tensile strength | Notched Izod | Deflection at 66 psi |
|---|---|---|---|---|
| Homopolymer | Propylene only | 5,400 psi | 1.2 ft-lb/in | 210 °F |
| Impact copolymer | Ethylene rubber phase | 3,800 psi | 12.5 ft-lb/in | 190 °F |
| Random copolymer | Ethylene in the chain | Not on this sheet | Not on this sheet | Not on this sheet |
Those figures come from one distributor’s polypropylene property page, which lists both grades on the same test methods.
Read the impact column again. One number is more than ten times the other, and both are sold as PP.
Now the part that surprises buyers. The tougher grade is the weaker one on paper, at 3,800 psi against 5,400. That is not a printing error.
The rubber phase gives way earlier under a slow pull, and it absorbs far more energy under a sudden hit. A crate wants the second behaviour, a shelf bracket usually wants the first.
Random copolymer is the grade the table cannot settle, because the two distributors we could read did not list it. It is the clear one, and clarity is usually why it is chosen.
When a buyer asks for a clear part, a random copolymer is one answer. The copolyester sold as a clear alternative is the other, and the two sit at other price points.
One more number belongs in a quote. Melt flow rate is measured at 230 degrees Celsius under a 2.16 kg load. The figure means nothing without that condition attached.
A sheet and profile grade sits around 0.5 grams per ten minutes. The grades used in the shrinkage trials below ranged from 8 to 35 on the same test.
Same family, same test, a spread of seventy times. A quote that says only PP has told you nothing yet.
The Number That Decides The Tool
Every thermoplastic shrinks as it cools. Semi-crystalline resins shrink more, because the chains pack into crystals and the crystals take less room than the melt.
PP is the extreme case in the commodity group. That is why its shrinkage deserves its own section.
The most useful data here comes from three Dow researchers. They moulded eight grades and presented the work at a conference. Plastics Today summarised it.
The trials used two plaque tools, and every part was measured a week later. Two findings matter for a buyer.
First, the base resins shrank between 0.013 and 0.022 cm/cm, which is 1.3 to 2.2 percent.
Second, the filled and compounded grades shrank between 0.005 and 0.010, or 0.5 to 1.0 percent. Adding filler or rubber cut the movement by about half.
A moulder’s shrink rate chart prints a wider band for the family, 1.0 to 3.0 percent. That is not a disagreement. One is a measured set of plaques, the other a production range.
| Source | Grades measured | Shrinkage, cm/cm | As a percentage |
|---|---|---|---|
| Dow trials, 1999 | Reactor grade, unfilled | 0.013–0.022 | 1.3–2.2 % |
| Dow trials, 1999 | Compounded, filled or rubber | 0.005–0.010 | 0.5–1.0 % |
| Moulder’s chart | Family range | 0.010–0.030 | 1.0–3.0 % |
Put a number on that. A 200 mm dimension on an unfilled grade at 1.8 percent moves about 3.6 mm.
Split the allowance across both sides and the steel still has to be cut 1.8 mm long per side. Get it wrong and no dial on the press can fix the part.
The trials also give four sensitivities, each with its own unit. These are the levers a moulder has after the tool exists.
Shrinkage rises by 0.001 per 0.4 mm of added wall thickness. It falls by 0.001 per 6.9 megapascals of cavity pressure.
It falls by 0.001 per 27.8 degrees of added melt temperature, and rises by 0.001 per 18.3 degrees of added mould temperature.
A moulder’s guide puts it as a rule of thumb. A 10 percent change in mould temperature moves shrinkage by about 5 percent of its own value.
Two more facts from the same work decide part design. Shrinkage grows slightly with flow length, by 0.0005 over 13 cm.
And cross-flow shrinkage is generally greater than shrinkage along the flow. That difference, not the average, is what turns a round bore into an oval one.
The practical rule that follows is simple. Never accept a single shrinkage figure on a quote, and never let a supplier promise a tolerance before the tool is cut.
Ask for the grade name, the filler content, the wall thickness the figure refers to, and whether it is flow or cross-flow. Four answers, one line each.
Wall Thickness, Ribs And Warpage
Shrinkage is not a single number for a part. It varies with the section, and the section is drawn before the tool is cut.
The trials give the link directly. Every extra 0.4 mm of wall adds about 0.001 of shrinkage, which is one tenth of a percentage point.
Go from a 1.5 mm wall to a 3 mm wall and the figure can climb by nearly half a point. On a 150 mm panel that is most of a millimetre.
Now put a thick boss beside a thin wall. The thick section cools last, keeps shrinking after the thin one has set, and pulls the flat face with it.
The same arithmetic explains a sink mark. A rib drawn at full wall thickness is a thick section, so the face above it sinks.
A rib at half the wall is the usual compromise. The section stays thin enough to cool with the wall. The rib still adds stiffness, because stiffness grows with the cube of depth.
Warpage comes from the other finding. Shrinkage across the flow is bigger than shrinkage along it, so a flat panel pulls into a curve as it cools.
Three things reduce it, and all three are cheaper before the tool exists. Keep the wall even. Put the gate where flow runs the same distance both ways. Use a filled grade if the part can take the loss of impact strength.
Then agree how the part will be measured. The trials took readings a week after moulding, because nothing moved after the first two days.
That detail settles arguments. A part measured an hour after ejection is still cooling. A supplier who measures that way will always look better than the tool really is.
Write the timing into the drawing: measure 24 hours after moulding, at 23 degrees, on the datum the drawing names.
Three Temperatures That Get Mixed Up
Search for a service temperature for this resin and three answers come back. They are three different measurements, and only one belongs on a drawing.
Melting point. The US food contact rule prints 160 to 180 degrees Celsius for the PP item it covers, and a homopolymer sheet datasheet prints 163.
That is the temperature at which the crystals come apart. It is a processing fact, not a working limit, and a part at that temperature is a puddle.
Heat deflection. A bar is loaded and heated, and the figure is the temperature at which it bends a set amount. For the homopolymer it is 210 Fahrenheit at 66 psi, about 99 degrees Celsius.
The copolymer reads 190 Fahrenheit, about 88 degrees Celsius, on the same test. Lower stiffness shows up as a lower deflection temperature.
Continuous service in air. The same data page gives 180 Fahrenheit, about 82 degrees Celsius, as the long-run limit in air for the homopolymer.
That is the number for a part that has to hold its shape for years. It is roughly half the melting point, which is the normal gap for a semi-crystalline plastic.
Two trade pages disagree with both. One tank supplier gives 100 to 130 degrees Celsius continuous, then states 0 to 180 Fahrenheit for its own tanks on the same page.
A resin blog gives 100 to 110 degrees Celsius as the long-run ceiling. Both pages are selling something, and neither prints a test method.
The cold end is less argued. Below 0 degrees Celsius this resin becomes brittle, and that is where a homopolymer lid cracks in a cold lorry.
So a drawing note should name one figure and one test. Continuous service at 82 degrees Celsius in air is a sentence a supplier can be held to. A melting point is not.
One consequence follows for packaging. A container sold for hot fill or for a warming cabinet needs a rating for that use. The grade has to say so.
That question leads straight to the next one, because heat and food contact are the two claims buyers check hardest.
What Food Grade Polypropylene Means
There is no certificate called food grade. The phrase is a claim about a finished part, made against a written rule, and the rule has a number.
In the United States the number is 21 CFR 177.1520, titled olefin polymers. PP is defined there as a basic polymer made by the catalytic polymerization of propylene.
The section then prints a table of items. Each item gives a density window, a melting point window and a limit. The limit fixes how much of the polymer may come out of the finished part.
The text of the section is short enough to read in one sitting, and most of the surprises are in that table.
Item 1.1a covers PP itself. Density 0.880 to 0.913, melting point 160 to 180 degrees Celsius, and a maximum extractable fraction of 6.4 percent in n-hexane.
There is a second limit on the same row: no more than 9.8 percent may dissolve in xylene at 25 degrees Celsius. That number measures the part of the resin that is not crystalline.
Now the split that most supplier declarations miss. Copolymers get their own items, and the item depends on what the part will hold.
An olefin copolymer for ordinary food contact sits under item 3.1a, with a limit of 5.5 percent in n-hexane at 50 degrees Celsius.
An olefin copolymer for packing or holding food during cooking sits under item 3.2a, and there the limit is 2.6 percent at 50 degrees Celsius.
| Item | What it covers | n-Hexane limit | Test condition |
|---|---|---|---|
| 1.1a | Polypropylene | 6.4 % | Reflux, 2 hours |
| 3.1a | Copolymer, no cooking use | 5.5 % | 50 °C, 2 hours |
| 3.2a | Copolymer for cooking | 2.6 % | 50 °C, 2 hours |
Do not rank those three numbers as if they sat on one scale. The PP row is tested at reflux, where n-hexane is near its boiling point. The copolymer rows are tested at 50 degrees.
The test itself is described in the same section. A sample is refluxed in the solvent for two hours and filtered at the boiling point. The filtrate is then evaporated and the residue is weighed.
That is the whole idea. Take the finished article, cook it in a solvent that stands in for fatty food, and weigh what comes out.
Europe answers the same question with another instrument. The plastics regulation numbered 10/2011 sets an overall migration limit of 10 milligrams per square decimetre of contact surface.
For food for infants and young children the limit is written per kilogram instead, at 60 milligrams. The recitals explain that figure: it is what a one kg cube of food would see at the surface-to-volume ratio of a cubic pack.
So the American question is how much polymer comes out in a named solvent. The European question is how much total mass moves into a set of food simulants.
Both are tests on the finished part. Neither is settled by the name of the resin, and neither is settled by the word on the box.
One claim is worth correcting, because it appears on every consumer page. PP is described as BPA free, which is true for a dull reason: there is no bisphenol anywhere in a propylene chain.
The question that matters is what else went in. Antioxidants, acid scavengers, slip agents and colour carriers are added to the resin, and those are the substances a migration test is looking for.
Two practical notes also belong here. The resin takes up almost no water, so a food container holds its size in a humid store.
And the European framework rule on food contact materials is separate from this one. A supplier who answers a PP question with that framework has answered another question.
A rubber part takes another route. The silicone rubber route through the same question uses its own limits and its own test.
What Polypropylene Is Bad At
Most sourcing problems with this resin come from asking it to do something it was never rated for. Five limits cover nearly all of them.
Sunlight. Unstabilised PP chalks and then cracks outdoors. Titanium dioxide or carbon black in the compound is what holds it together.
A garden chair and a hidden bracket can use the same resin and need other additive packages. Ask which package is in the grade, not whether it is UV stable.
Gluing and printing. The same data page that prints the strength figures lists difficult to bond, and difficult to print or paint, as known weaknesses.
Low surface energy is the reason. Ink and adhesive sit on the surface instead of keying into it, so a decorated part needs a surface treatment step on the drawing.
Cold. Below 0 degrees Celsius the homopolymer goes brittle. A part that must survive a freezer or a winter lorry is a copolymer question.
Stress and chemicals together. Either one alone may be fine. A stressed part in contact with a solvent, a detergent or a fatty product can crack while it sits there.
Strong oxidisers. It holds up to acids, bases and most organic solvents, and not to strong oxidising agents. Cleaning agents are where this bites.
None of those five is a reason to avoid the material. Each one is a line that has to reach the specification before the sample is approved.
Six Lines For The Order Sheet
Everything above becomes useless unless it reaches the spec. These six lines are the ones that keep coming back as disputes.
One, the grade and the flow rate. Name the maker’s grade, then the melt flow rate with its condition. That means 230 degrees Celsius, a 2.16 kg load, and the method, ISO 1133 or ASTM D1238.
Add a tolerance. A band of plus or minus 15 percent on flow rate is common, and without a band the test becomes a suggestion.
Two, the shrinkage allowance. Put the figure on the drawing, with the wall thickness it refers to and whether it is flow or cross-flow.
Then name the trial that proves it: five shots from the production tool, measured 24 hours after moulding, at 23 degrees, on the drawing datum.
Three, the food contact item. Write the citation, not the claim. Item 1.1a for a homopolymer in the United States, item 3.1a or 3.2a for a copolymer, and the European figure where that market applies.
Ask for the extractive result on your part. The report has to describe the article that ships, and a report on a test plaque is another object.
The wider map of these duties sits in this site’s guide to how the rules divide by material. A silicone part follows a separate rule again.
Four, the additive package. Say whether the part needs UV protection and heat stabilisation, and name what is allowed to deliver it.
Colour belongs in the same line. A masterbatch carrier that is not compatible with the base resin is a common cause of dull patches and weak welds.
Five, regrind and colour. State the share of regrind allowed in the shot, and whether regrind from another colour may be used as core resin.
Regrind shortens the chain, and a shorter chain flows faster and shrinks differently. If the answer is not on the sheet, it is decided at the machine.
Six, the tool. Record who owns the mould, who stores it and what happens to it if the order stops. A shrinkage correction after trial is the moment that clause matters.
That last line connects to cost. What the mould itself is likely to cost depends on the number of cavities and the steel, not on the resin. The resin does decide how much correction the steel will need.
Ownership is a separate argument with its own paperwork, covered in this guide to who holds a custom tool.
All six lines fit on one page, which is the point. The one-page sheet a factory works from is the format that survives the trip from sales desk to press.
For a container programme, add the wall and stacking figures from this site’s guide to sourcing plastic containers. Shrinkage and stack load are the two numbers that decide whether a crate keeps its shape.
Send the drawing and the resin grade you were quoted, with the wall thickness marked on it. I will check the shrinkage allowance against that grade, confirm which food contact item the part can cite, and list what to fix before the steel is cut. No cost, no obligation.
Check My DrawingQuestions Buyers Ask
Is polypropylene food safe?
A part made from covered resin, tested on the finished article, usually is. The name of the plastic proves nothing, because the limits are set per item and measured on the part.
Why did my polypropylene part crack in the cold?
You are probably holding a homopolymer. Below 0 degrees Celsius it turns brittle, and the impact copolymer is the grade that keeps its toughness in a freezer.
Can polypropylene be glued or printed without a treatment?
Usually not, and the property pages say so. Its surface gives ink and adhesive little to grip, so a decorated part needs a treatment step written into the process.
Is polypropylene recyclable?
It melts and re-forms, and it carries the number 5 in the resin code. What limits it in practice is sorting and food contamination, not the chemistry.
Does polypropylene take up water?
Almost none, which is why a container keeps its size in a damp store. Water absorption is listed as slight on the property sheets rather than as a percentage worth planning around.
Polypropylene or polyethylene for a crate?
Polypropylene is stiffer and takes more heat, so it holds a shape under load. Polyethylene is tougher at low temperature and easier to weld, which is why tanks often use it.
Questions & Comments
We read every one and reply within 24 hoursIf a polypropylene quotation lands on your desk, send the grade name and the wall thickness with it. I will say which shrinkage figure applies and which food contact item the part can actually cite.